The main reason why the resistance value of the switch line is too large:
The silver paste was not sufficiently stirred before printing.
The line baking time is insufficient after printing, and the temperature is low.
The selected wire mesh is too fine.
The silver paste of the printed circuit is too thin.
The silver paste is too thin, and too much thinner is added, so that the silver content is too small or a non-silver paste special thinner is used.
The line graphic design is unreasonable.
The quality of raw materials such as silver paste is not good.
Before printing, make sure that the silver paste is fully stirred. When adding the silver paste, it must also be fully stirred.
Master and control the baking time and temperature.
Replace the screen with coarser mesh to make a qualified screen
To change the plate-making method, consider using a thick plate.
Check the concentration of silver paste, pay attention to control the addition of thinner, and ensure that the thinner matching with the silver paste is used.
Check whether the circuit design is reasonable, and make necessary improvements to the designed circuit.
Replace the raw materials such as silver paste that meets the requirements.
You must now have a certain understanding of tactile and non-tactile switches. Membrane switch is a very good electronic accessory, widely used in medical, military, marine, and agricultural, etc. Niceone-tech can provide various types of touch keypad membrane keyboards/switches. If you need to customize the membrane switch, please feel free to contact us, our contact information is info@niceone-tech.com.